Blu User Guide
Blu is developed to be a strong resin that has a high resolution, precision, and is easy to print. It is tough and hard enough for making functional parts yet easy to print and clean for general use.
And it should not stink up the user's work environment.
Due to the higher polymer content for its outstanding mechanical properties, the ideal printing condition for Blu is over 25C.
If user can maintain a resin temperature of 30C, the printing time could be further reduced.
Please download profiles here based for Elegoo, Anycubic, Phrozen, Peopoly, EPAX, Creality: Click here to download profiles
Check out recommended support settings if you have print failures
Exposure For Blu and Blu Clear V2 (Not Blu Obsidian Black, Not V3)
Recommended |
Resin Temperture 25-35C
|
Room temperature 20-28C
|
||||||||||
Printer | Layer Height | Exposure (s) | # of Initial Layers | Exposure for Init Layers | Exposure (s) | # of Initial Layers | Exposure for Init Layers | Note | ||||
Photon | 50um | 11-12 (s) | 4 | 60 s | 12-13 (s) | 6 | 90 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Photon-S | 50um | 10 (s) | 4 | 60 s | 11 (s) | 6 | 75 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Photon Mono | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Photon Mono X | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
LD-002R | 50um | 10 (s) | 4 | 40 s | 11 (s) | 4 | 50 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
EPA X1 | 50um | 10 (s) | 4 | 55 s | 10 (s) | 6 | 75 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
EPA X1 | 100um | 12 (s) | 4 | 75 s | 12 (s) | 6 | 90 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Elegoo Mars | 50um | 11 (s) | 4 | 50 s | 11 (s) | 6 | 60 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Mars 2 Pro | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Mars 3 | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Saturn | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Shuffle | 50um | 9(s) | 5 | 75 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | |||||||
Shuffle XL | 50um | 12(s) | 5 | 75 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | |||||||
Sonic Mini 4K | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Might 4K | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Mega 8K | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
D7 | 50um | 9(s) | 5 | 75 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | |||||||
Inkspire | 50um | 11s | 4 | 50 s | 12-13 (s) | 6 | 90 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Moonray | 50um |
use settigs for nextdent Ortho rigid
|
use settigs for nextdent Ortho rigid
|
|||||||||
Sonic Mini | 50um | 4s | 5 | 35s | 4s | 5 | 35s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Slash | Siraya on the Slash is better than anything I’ve tried...and I’ve tried 5-6 other resins on the Slash. Example from left to right are 100um, 75um, and 50um. The one I’m holding is 50um. 100um 5 sec 75um 4 sec 50um 3.5 sec 25um 2.8 sec 10um 2.5 sec - LED power 250 (default) - First layer for all 12sec/ first 3 layers (default amount). - Slow setting for Lift speed - 8mm lift height is safest and allow time resin to flow back (they only allow you to pick from 3,8, and 15mm height...which sucks...I'd like 6mm if I could. - Cooldown between layers on auto (smaller prints i do 2sec to speed things up) - Supports point(head) size no less than 1mm, but 1.5 is recommended with 2mm shaft. |
Exposure For Blu Obsidian Black and for Blu V3
Recommended |
Resin Temperture 25-35C
|
Room temperature 20-28C
|
||||||||||
Printer | Layer Height | Exposure (s) | # of Initial Layers | Exposure for Init Layers | Exposure (s) | # of Initial Layers | Exposure for Init Layers | Note | ||||
Photon | 50um | 9.5 (s) | 4 | 60 s | 9.5 (s) | 4 | 60 s | 6mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Photon-S | 50um | 7.5 (s) | 4 | 50 s | 7.5 (s) | 4 | 50 s | 6mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Photon Mono | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Photon Mono X | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
LD-002R | 50um | 9 (s) | 4 | 40 s | 9 (s) | 4 | 50 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
EPA X1 | 50um | 9 (s) | 4 | 55 s | 9 (s) | 4 | 55 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Elegoo Mars | 50um | 9.5 (s) | 5 | 45 s | 9.5 (s) | 5 | 45 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Mars 2 Pro | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Mars 3 | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Saturn | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Shuffle | 50um | 9(s) | 5 | 75 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | |||||||
Shuffle XL | 50um | 12(s) | 5 | 75 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | |||||||
Sonic Mini 4K | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Might 4K | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
Mega 8K | Where to find printer profiles: https://drive.google.com/drive/folders/1eCz4_dc0fT-jfBLp4L9mKYebY90lfHHO?usp=sharing | |||||||||||
D7 | 50um | 8(s) | 5 | 65 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | |||||||
Inkspire | 50um | 10s | 4 | 50 s | 10s | 4 | 50 s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface | ||||
Moonray | 50um | use settigs for nextdent Ortho rigid | use settigs for nextdent Ortho rigid | |||||||||
Sonic Mini | 50um | 3s | 5 | 30s | 3s | 5 | 30s | 10mm lift distance help, lift speed 40mm/min, with support facing side surface |
Exposure For Blu Nylon Black Only
Make sure the support tip diameter is 1.2mm for larger prints with a depth of 0.5mm. See more full settings recommended
https://www.facebook.com/groups/sirayatech/permalink/290257771885611/

It is best to use island style base like below left, not the raft style on the right. If you have a problem keeping the first layer on, make sure you level again to minimize gap between build plate and LCD screen
Cleaning:
Use a painter brush (or any brush made with hair) remove excess resins on the printed part with Use 95% concentrated Ethanol (preferred) or IPA to clean. Some form of methnol should work but make sure it does not contain acetone.
Do not submerge the parts in alcohol for more than 5 minutes. After cleaning remove alcohol as soon as possible with a hair dryer or air blower. For complex part with lots cavities, it may be a good idea to clean/dry multiple times.
Users can check by touching the dried surface of the part to see if it is still sticky. If the dried surface is still sticky, wash some more and dry again.
Post Curing:
Blu reached its optimal strength when the printed part is post-cured with UV after cleaning. Use 395-405nm UV light and cure for about 15 minutes.
Make sure the resin is completely cleaned off and there is no alcohol left (it needs to be dry) on the print before curing.
Curing by submerging objects in water will significantly increase curing efficiency
For Biocompatibility related applications, please follow the post-processing guidelines here:
https://siraya.tech/blogs/news/blu-biocompatibility-certification-iso-10993
Blu Mechanical Properties(Emerald Blue, Clear V2, V3, Obsidian Black)
Shore D 85
Tensile Strength 50Mpa
Young’s Modulus 1800Mpa
Elongation At Break: 32%
Heat Deflection Temperature: 75C
Shrinkage 1%
Viscosity 700 CPS
MSDS
https://drive.google.com/open?id=1QA9HKiQD-9b4onVCs1W_MjBiT940yGOk
Blu Nylon Black Mechanical Properties
Shore D 80
Tensile Strength 60Mpa
Young’s Modulus 2000Mpa
Elongation At Break: 40%
Heat Deflection Temperature: 70C
Shrinkage 1%
Viscosity 750 CPS
MSDS